Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Determination of Flexural Strength of Concrete: Standards, Test Methods, and Applications

Concrete flexural strength testing (modulus of rupture) is a fundamental mechanical test that determines the ability of hardened concrete beam specimens to resist bending failure. This article explains the determination of flexural strength of concrete in accordance with international standards such as ASTM C78, EN 12390-5, ISO 1920-4, and GB/T 50081, covering specimen requirements, testing procedures, calculation formulas, and typical engineering applications.

Technical Overview

Flexural strength, also known as modulus of rupture (MOR) or flexural tensile strength, is the maximum stress that a concrete beam specimen can withstand before failure when loaded in bending. Because plain concrete is a brittle material with low tensile capacity, flexural strength is a critical design parameter for structures where bending and tension govern performance, such as concrete pavements, industrial floors, slabs-on-grade, and airport runways.

The determination of flexural strength is performed by loading a prismatic concrete beam to rupture under a controlled loading configuration, typically third-point loading or center-point loading. The test is standardized internationally by ASTM C78/C78M (third-point loading), ASTM C293/C293M (center-point loading), EN 12390-5, ISO 1920-4, and GB/T 50081. For ordinary structural concrete, flexural strength typically ranges from approximately 3.5 MPa to 6.0 MPa, generally about 10% to 20% of the corresponding compressive strength.

  • Flexural strength characterizes the tensile behavior of concrete under bending stress
  • It is the primary acceptance index for cement concrete pavement construction
  • Results are used for mix design optimization, quality control, and structural evaluation

Testing Samples

Standard Prismatic Beam Specimens

The standard test specimen is a rectangular prism cast with its long axis horizontal. Common specimen dimensions include 150 mm × 150 mm × 550 mm or 150 mm × 150 mm × 600 mm beams under GB/T 50081 and EN 12390-5, and 152 mm × 152 mm × 508 mm (6 in. × 6 in. × 20 in.) beams under ASTM C78. The support span is typically three times the specimen depth, for example 450 mm for a 150 mm deep beam. Smaller 100 mm × 100 mm × 400 mm or 100 mm × 100 mm × 500 mm prisms may be used when the maximum aggregate size does not exceed approximately 25 mm, although size-effect corrections may be required.

Specimen Preparation and Curing

Beams are cast in rigid, watertight steel or cast-iron molds and compacted by internal vibration or tamping in accordance with the applicable fresh concrete sampling and specimen preparation standards. Specimens are demolded after 24 hours and stored under standard moist curing conditions at 20 ± 2 °C with relative humidity above 95% until the specified test age, typically 28 days. Prior to testing, beams are removed from the curing water, wiped to a saturated surface-dry condition, and tested without unnecessary delay to prevent moisture loss.

Sampling Requirements

A minimum of three beam specimens is generally required for each concrete batch, mix design, or test age to obtain a representative mean value. Specimens should be free from visible defects, and cross-sectional dimensions are measured at the fracture location to an accuracy of 1 mm before testing.

Testing Items

The core testing item is the determination of flexural strength (modulus of rupture) of hardened concrete at a specified age. Related evaluations commonly performed alongside or derived from the test include:

  • Flexural strength (modulus of rupture) of beam specimens at 7, 28, or other specified ages
  • Conformity assessment against specified design flexural strength grades, for example 4.0 MPa, 4.5 MPa, or 5.0 MPa for pavement concrete
  • Quality control and acceptance testing of ready-mixed and site-batched concrete
  • Performance characterization of fiber-reinforced concrete and pavement mixes
  • Statistical evaluation of strength uniformity for construction quality assessment

Testing Methods

Third-Point Loading Method (Four-Point Bending)

The third-point loading configuration, specified in ASTM C78/C78M and GB/T 50081, applies two equal point loads at the third points of the support span. This arrangement produces a region of constant maximum bending moment, free of shear, between the two loading points, making failure less dependent on localized weaknesses. The flexural strength is calculated as: f = F·L / (b·h²), where F is the maximum applied load, L is the span length between supports, and b and h are the average width and depth of the specimen at the fracture section.

Center-Point Loading Method (Three-Point Bending)

>The center-point loading configuration, specified in ASTM C293/C293M and permitted under EN 12390-5, applies a single concentrated load at midspan. The maximum bending moment occurs only at one cross-section, so results tend to be slightly higher and more variable than third-point loading. The flexural strength is calculated as: f = 3F·L / (2·b·h²).

General Test Procedure

  • Measure and record the specimen width and depth at midspan and near the supports
  • Center the beam in the loading frame and align the loading and support rollers parallel to the specimen faces
  • Apply the load continuously and uniformly without shock using a calibrated compression or universal testing machine fitted with a flexural attachment
  • Maintain the specified loading rate: approximately 0.014 to 0.021 MPa/s extreme fiber stress increase under ASTM C78, or 0.05 to 0.08 MPa/s under GB/T 50081
  • Record the maximum load at fracture and mark the exact fracture location on the specimen
  • Calculate the individual flexural strength value and determine the mean of the valid specimens

Result Validity and Reporting

Under third-point loading, the fracture must occur within the middle third of the span for the result to be considered fully valid. If the fracture occurs outside the middle third by more than 5% of the span length, the result is discarded and a retest is performed. The test report should include specimen identification, dimensions, curing history, test age, loading configuration, individual and mean flexural strength values, fracture location, and any observed defects or deviations from the standard procedure.

Applications

Flexural strength determination is essential wherever the bending resistance of concrete controls design, durability, or acceptance. Typical applications include:

  • Quality control and acceptance testing of cement concrete pavements for highways and expressways
  • Construction supervision and acceptance of airport runways, taxiways, and apron pavements
  • Performance verification of industrial floors, warehouse slabs, and bridge deck overlays
  • Evaluation of fiber-reinforced concrete and special pavement mixes in accredited third-party laboratories
  • Concrete mix design optimization and strength grade verification by ready-mix producers
  • Research on fatigue behavior, durability, and tensile performance of cement-based materials

FAQ

What is the difference between flexural strength and compressive strength?

Compressive strength measures the resistance of concrete to crushing loads, while flexural strength measures its resistance to bending and cracking under tension. Compressive strength is used for most structural design, whereas flexural strength is the governing acceptance index for pavements and slabs where traffic loads induce bending stresses.

Can flexural strength be estimated from compressive strength?

Yes, empirical relationships are commonly used, with flexural strength approximately equal to 0.6 to 0.8 times the square root of the compressive strength in MPa. However, such estimates are indicative only, because flexural strength is strongly influenced by aggregate type, moisture condition, and curing quality. Direct beam testing remains the preferred method for acceptance decisions.

Why must the fracture occur within the middle third of the span?

In third-point loading, only the middle third of the span experiences the constant maximum bending moment. A fracture outside this region indicates failure at a lower stress zone, often due to a local defect or stress concentration, so the calculated value would not represent the true flexural strength and the result is discarded.

Which loading method is preferred for pavement acceptance testing?

Third-point loading (ASTM C78 or GB/T 50081) is generally preferred because it produces a uniform bending moment zone, yields lower scatter, and better represents the stress distribution under traffic wheel loads.

How many specimens are required and how is the result evaluated?

A minimum of three beam specimens is tested, and the mean flexural strength is compared with the specified design value. Individual values that deviate excessively from the mean by more than 15% are typically excluded from the average in accordance with the applicable standard requirements.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing